OF DECAY COMPARTMENTALIZATION JW* IN TREES *H2. \v fa*** Agriculture Information. U.S. Department of Agriculture. Forest Service. Bulletin No.

Similar documents
CABLING AND BRACING. January 1980, Vol. 6, No. 1. by Alex L. Shigo and Robert Felix

TREES AND TREATMENTS. Alex L. Shigo Forester, Northeastern Forest Experiment Station Durham, NH

Internal Defects Associated with Pruned and Nonpruned Branch Stubs in Black Walnut

Detection of Active Decay at Groundline in Utility Poles

Com partmen tal izat ion of Decayed Wood

Building Bigger Things

Wood structure I: Basic features, structure and cell types

What materials are available?

NWFA/NOFMA International Standards for Unfinished Solid Wood Flooring

Challenges of Oak Timber - Pests.

Wood anatomy. 600 Wood anatomy

Wood & Timber. Wood & Timber

Exam Sheet, Part 1. hardwood softwood. pith, heartwood, sapwood, vascular cambium, phloem, outer bark. sapwood, phloem, vascular cambium, outer bark.

NOFMA GRAIN DESCRIPTIONS OAK PLAIN SAWN QUARTER SAWN RIFT SAWN QUARTER/RIFT SAWN

!DETECTION OF COMPRESSION FAILURES IN WOOD

VARIATION IN THE DECAY RESISTANCE BETWEEN SAPWOOD AND HEARTWOOD OF Parashorea malaanonan. Mahmud Sudin & Razak Wahab

Attachment A BURLINGTON NORTHERN SANTA FE SPECIFICATIONS FOR CROSS TIES AND SWITCH TIES I. GENERAL

Sawn timber grading in Lao PDR. Product grading manual: rules and recommendations

Macroscopic and microscopic aspect of abiotic wood decomposition

NATIONAL GRADING RULE FOR SOFTWOOD DIMENSION LUMBER INTERPRETATIONS

Recommended Resources: The following resources may be useful in teaching this

Timber Check Moisture Meter

TIMBERS BEAMS & STRINGERS, POSTS & TIMBERS

Kapur (Dryobalanops Aromatica)

Guide to the identification of UK wood-boring insects

Basic Guide to Identification of Hardwoods and Softwoods Using Anatomical Characteristics

Wood Properties Important to Exterior Coating Performance

DEFINITIONS 702. BURL - A distortion of grain, usually caused by abnormal growth due to injury of the tree. The effect of burls is assessed in relatio

Comparison of Methods to Determine Disk and Heartwood Areas

Decay and Termite Resistance of Western Juniper Sapwood and Heartwood Under Tropical Conditions

FLUSH WOOD DOOR AND MODERN JAMB SPECIFICATION GUIDE

FACTORY-FINISHED STAINED WOOD DOORS

Chapter 2 Basic Properties of Undervalued Hardwoods. John I. Zerbe Volunteer, USDA Forest Products Laboratory. Properties of Soft Maples

Grading Of Oak: We are very different than any of our competitors and the details below explain how we grade our raw material.

Inspection of timber construction by measuring drilling resistance using Resistograph F300-S

Beech, American American Beech grows in Canada and the United States. It contains white sapwood and reddish heartwood with a closed, straight grain. A

About wood. Forests NSW Commercial Services. What is wood?

Wood structure II: Anatomy and properties

American Woodcock. SONG A nasal beeping peent heard. FOOD Mostly earthworms; also eats. FUN FACT The American woodcock is HABITAT.

GREAT OUTDOORS B. ACHIEVEMENT DAY REQUIREMENTS Knot Display 40 Tree Disk 30 Special Project Marks EXHIBITION REQUIREMENT

Acecap/Medicap Application Guide:

Wood. Wood construction

NREM 1213, INTRODUCTION TO WOOD PROPERTIES AND WOOD PRODUCTS

TABLE OF CONTENTS USER MANUAL. ÓAllison Tree, LLC 1830 Sugar River Road Verona, WI allisontree.com

SPECIFICATIONS FOR TIMBER CROSSTIES (Latest Revision as of January 2014)

PATTERN OF VARIATION OF FIBRIL ANGLE WITHIN ANNUAL RINGS OF PINUS ATTENURADIATA

Rx for MACHINING WOOD. Gene Wengert & Bobby Ammerman

(elpe-* EFFECTS Of TENSION WOOD IN HARDWOOD ILUMI3ER AND VENEER iliri II n mi1 iriinuirliir [Riau

PiCUS Tree Tomography Methods at a Glance

Appearance grading / European standard EN Strength class / French standard NFB

4-H Wood Science Leader Guide. Basic Information About Wood

Fastener Hole Crack Detection Using Adjustable Slide Probes

v t industries VENEER GUIDELINES


Bark Craft MAKE YOUR OWN ROUND BIRCHBARK CONTAINER. By Beke Olbers EXTRA Survival & Bushcraft THEBUSHCRAFTJOURNAL.COM 00. Photo - extrasurvival

Recommended Resources: The following resources may be useful in teaching this

APPENDIX A. WOOD CHARACTERISTICS. Structure of Wood

Suwanee Lumber Specialty Woods

Woven Wire Fence. Fencing for small ruminant prescribed grazing. Job Sheet No. AL382C - 1

Installation : EB TY Invisible Fastener or Screwed Down Structural Deck BS 8201:1987 maximum span of joists is 600 mm

Strength Grading of Hardwoods

Understanding the Characteristics of Wood

General Characteristics of Solidfloor TM engineered flooring

OBSERVATIONS ON THE ANATOMY OF THE CRICKET-BAT WILLOW (SALIX CAERULEA SM.) BY GEORGE METCALEE. The Botany School, Cambridge

GENERAL INFORMATION. Types of wood surface protection. Recommendations for the care of garden architecture products

WALL AND ROOF PLANK ALL WEST COAST SPECIES

STANDARD LIMITATIONS IN ACCORDANCE WITH CORPORATE STANDARD STO

Forest Structure and Bird Assemblages in Old-Growth and Managed Hemlock Hardwood Forests of the Western Laurentian Great Lakes Region, USA

Post Selection Post Selection

Appearance grading / European standard EN Strength class / French standard NFB

Measuring Tree Age Teacher Instructions

WOOD GOOD GOODWOOD.SX LUMBER PROFILE

ALAN CARTER STUDIO 5332 RIVERVIEW DR., LISLE, IL

Quality and Surface Modification of BC Softwood For Value-Added Products

Kansas Insect Newsletter

HOW GROWTH Of WHITE PINE AFFECTS ITS!PROPERTIES FOR MATCHES

Have a clear understanding of wood use classes

AIRCRAFT WOOD INSPECTION

Accoya Radiata Pine Lumber Grading Specifications. Grade Names & Definitions for Accoya Radiata Pine Version 8.2

Section 912. TIMBER AND LUMBER

Lesson: Feathers in the Forest

Korean standards of visual grading and establishing allowable properties of softwood structural lumber

Protocol for Tree Core Collection and Preparation for Ring. Width and Nitrogen Isotope Analysis

Field Trip to PATUXENT REFUGE

From Inside. A tree, or a part thereof, is something we all need at one point in time.

Lesson: Feathers in the Forest

Field Trip to PATUXENT REFUGE

Glass & Soil Analysis

Wood Preservation. Food in the form of cellulose, hemicellulose, or lignin. Chemically treated wood is not a food source.

The Owner's Guide to Piano Repair Focus On: Repairing a Separated Back on the Vertical Piano

LUMBER GRADING SPECIFICATIONS

Plain Sliced Cherry Standard Stains (SS1) #100 - Clear #175 - Barley #200 - Spiced Walnut #225 - Zin #250 - Copper #300 - Medium Brown #325 - Rose #35

NLGA INTERPRETATIONS

SOLIGNUM APPLICATION SOLIGNUM KOPPERS PERFORMANCE CHEMICALS

VOLUNTA PARKET. Welcome to our world, a world of the high quality wood, splendid colours and the most recent trends.

United States Standards for Grades of Dried Prunes

CAUSES OF BRASHNESS IN WOOD

10.2 Color and Vision

unsealed. Softwood walls, and have thin a hybrid of (creating

EVALUATION OF FUMIGANTS FOR DECAY CONTROL IN RED AND WHITE OAK TIMBERS. by T.L. HIGHLEY *

Transcription:

JW* COMPARTMENTALIZATION OF DECAY IN TREES \v fa*** *, *H2 8 v^ 'rr*u... Forest Service U.S. Department of Agriculture Agriculture Information Bulletin No. 405

Watercolor illustrations by David M. Carroll, Warner, New Hampshire. & U.S. GOVERNMENT PRINTING OFFICE : 1977 O 231-254 For sale by the Superintendent of Documents, U.S. Government Printing Office Washington, D.C. 20402

COMPARTMENTALIZATION OF DECAY IN TREES Alex L. Shigo Plant Pathologist, U.S. Department of Agriculture, Forest Service, Northeastern Forest Experiment Station, Durham, New Hampshire and Harold G. Marx Research Applications Staff Assistant, U.S. Department of Agriculture, Forest Service, Washington, D.C. Agriculture Information Forest Service Bulletin No 405 U.S. Department of Agriculture July 1977

INTRODUCTION The science of tree pathology emerged from studies on decay almost a century ago. Many of the concepts developed then have changed little over the years. But, in the last few decades some additional information on the decay process in trees has been developed. This new information has added to the basic story of decay without subtracting anything important from it. The new expanded concept of decay is simply more complete. And this new, more complete concept gives us a better opportunity to control decay. regulate and Dr. George H. Hepting made the first sound observations on compartmentalization of decay in trees in 1935. His ideas acted as a trigger for the work that followed. The work presented here is an expansion of his ideas. The information in this publication is based on 16 years of research by Dr. Shigo that involved complete dissections of approximately 10,000 trees mostly deciduous hardwoods, at least 1,000 conifers, and 17 tropical species. Details of these studies have been published elsewhere. The purpose of this publication is to show how most columns of discolored and decayed wood associated with trunk wounds in trees are compartmentalized. A great number of confusing terms are given to a wide variety of defects caused by discolorations and decays in trees. This book describes a system that makes it possible for forest managers to understand how most of these defects develop. To understand the system, the report must be studied very carefully. The system is called CODIT Compartmentalization Of Decay In Trees When the system is learned, it will act as the code for understanding a wide variety of defects on most tree species. The CODIT system is based on two major points. First, a tree is a highly compartmented plant. Second, after a tree is wounded, the resulting defects are compartmentalized. To apply the CODIT system it is necessary to understand that the new expanded decay concept developed in the last few decades includes: 1) Successions of microorganisms associated with discoloration and decay, and 2) Compartmentalization of discolored and decayed wood associated with trunk wounds. To begin with, decay of wood is a natural process caused by microorganisms, mainly fungi, that enter trees through wounds. Tree wounds are usually inflicted by fire, weather, insects, birds, small or large animals, or man and his activities. These wounds start the processes that can lead to decay, and decay is a major cause of damage to trees. While wood decay is most often caused by decay-causing fungi, these fungi are often intimately associated with bacteria and nondecay fungi in the process. Decay is the breakdown or decomposition of dead organic matter. It is also essential to new life. To understand how trees react to wounding and the associated defects by compartmentalizing the defects, it is necessary to reevaluate our concept of how a tree is constructed. A tree is considered here as a highly compartmented plant. In a sense, a tree is made up of many trees; each growth ring is a "tree." Each "tree" is divided into many compartments. A compartment can be thought of as a "room," with side walls made up of rays and front and back walls made up of cells that are the last to form in each growth ring. The top and bottom of the compartment is formed after wounding when the elements that transport liquids plug up. The compartment is the least common denominator of the tree. All the types of cells found in the woody stem of a tree will be found in each compartment. When microorganisms invade tree stems through wounds, they do so in successions. Bacteria, nondecay fungi, and decay fungi are often intimately associated in this invasion process. When microorganisms invade, they first surmount the chemical protective barriers set up by the tree and then move into the tree from compartment to compartment. The weakest walls of a compartment are the tops and bottoms, and the inner walls. The side walls are fairly strong. When all these walls fall to the invading microorganisms, there is another wall that begins to form. The wall formed by the cambium after wounding is zone. This wall the barrier confines the invasion to the wood present at the time of wounding. The new "trees" or rings that continue to form are then protected from invasion unless new wounds are inflicted. When new wounds are inflicted at later times, multiple columns of defect develop. An understanding of CODIT will help to clarify many misconceptions about decay.

Decay is a natural process. The breakdown of dead organic matter is essential for new life. Fungi are the major group of microorganisms that decay wood In many cases fungi accomplish this only in association with other organisms, especially bacteria.

Wood-inhabiting microorganisms enter trees through wounds Wounds start the processes that can lead to decay. And decay is a major cause of damage to trees. Decay

Conifers.Sound heartwood *M Well-healed.branch stubs.?-.. No large wounds High-quality pine developing

cdeciduous hardwoods and tropical trees Poorly healed branch stub Central column of discolored wood Well-Healed.branch stubs Open wound Clear, sound sapwood No heartwood ~ xbigh-qua!ity mapfe developing developing ity n>

Some common wounding agents are a-w-f X/' ~> 1 / Birds

Large animals

'- But, before explaining how wounds start the decay process, it/s necessary to understand... it»ow a tree is constructed. A tree ' *1Al <* is a highly compartmented planar, v *. Trees do not replace injured tissues as animals do. T "^compartmentalize injured tiss v»**v 'J y *'\S~ A tree is a - compartmented plant ttrt>crm-i! /»/, 10

In a sense, a tree is made up of many trees. Each growth ring can be thought of as a separate tree. Diagrammatic drawing of a tree. 'tree ^ x

In a diagrammatic way, here is how a tree is constructed. (The drawings are designed to give a general impression of compartments in trees and they are not intended as technical anatomical descriptions of cell types and arrangements.) The rays define the side walls of the compartments. The last few series of cells in the growth ring define the inner walls. The compartment has holes in the top and bottom walls because the flow of materials is maintained in a vertical direction. But, one of the first events that happens after wounding is a plugging of this system above and below the injury. Complete tops and bottoms then begin to develop on the compartments. (The term "walls" is used here in a very loose sense only to give the mental impression of "rooms" or compartments in the tree.) Pith Ray cells form side walls of compartments. 3 Last cells to form in growth ring form inner walls of compartment. 2 / Top and bottom of compartment form when vertical elements plug after wounding. 1 Compartment 12

In wood present at the time of wounding, the tops and bottoms of the compartments are the weakest walls. These we will call Wall 1. The inner walls are the second in weakness Wall 2. The side walls are fairly strong- Wall 3. The strongest wall is the one formed by the cambium after wounding Wall 4. Wall 1 is incomplete in living sapwood because the conducting elements vessels, tracheids conduct liquids in a vertical direction. But as heartwood forms, or after wounds are inflicted, pits close or the conducting elements are plugged. The rate and degree of pit closure and element plugging depend on many factors. Completion of Wall 1 is the result of a dynamic process. The plugging will set the limits for the vertical then extension of each compartment. When plugging occurs rapidly, short compartments form, but when plugging is slow, long compartments form. Wall 2 is continuous around every growth ring, and from the top to bottom of the tree. Wall 3 is discontinuous because sheets of ray cells are not continuous radially and longitudinally throughout the tree. Wall 4 is a much stronger, more localized version of Wall 2. The area longitudinal, tangential covered by Wall 4 will depend on many factors: Wound size, type, position, severity, time of year when wounding occurs, and intrinsic genetic potential to respond to wounds. Wall 2 is continuous around growth ring and from top to bottom of the tree. Compartment Side Walls 3 are the strongest walls. Present at time of wounding. Inner Walls walls. 2 are the next weakest Wall 1 is incomplete until heartwood forms or after wounding. It is not planar. Top and bottom Walls 1 are the weakest walls. Wall 3 is discontinuous. Sheets of ray cells may end abruptly both radially and longitudinally. Each growth ring is made up of many compartments. 13

Walls 2 are continuous around the rings and from top to bottom. A compartment Wall 1 is incomplete until after wounding Walls 3 are discontinuous inward and up and down. * j; \\ ^%k A compartment Vascular elements plug after wounding and complete Wall 1. 14

Discontinuous Walls 3 Continuous Walls 2 Each growth ring is made up of many compartments. A tree is a highly compartmented plant. Discontinuous Walls 3 Continuous Walls 2 15

Section B ection B Sectio i Barrier zone 10-year old wound on maple After wounding, the cambium forms Wall 4. This wall is called a barrier zone. It separates wood formed before wounding from wood that forms after wounding. Barrier zone Wall 4 formed after wounding Color key to all drawings RED Host response to wounding, chemical reactions to STOP invasion. GREEN Invasion processes by microorganisms GO through the barriers set up by the tree. BLUE Infection of dead and dying tissues on wound surface. BROWN Decay processes. 16

Pp3k?of bottom compartment Q^ner^WaM^2j Bark Section B Bark I: 1 4 Top and bottom walls are weakest walls Barrier zone equals strongest wall 2 Inner wall 3 Ray wall 17

Deep experimental drill wound Host response Maple After wounding, the tree reacts. Chemical barriers develop around the injured tissues. Some wood-inhabiting microorganisms surmount these barriers and begin to interact with the tree. The tree exerts a living protective force to keep the invaders out. and the invaders exert a strong force to get into the tree through the wound. When microorganisms are able to get in, they move from compartment to compartment. And when the walls of the compartments begin to fall to the force of the invaders, the tops and bottoms (Wall 1) go first, then the inner walls (Wall 2), and then the side walls (Wall 3). But, most of the time the barrier zone (Wall 4) holds, and confines the invaders to the wood present at the time of wounding. The figures 1, 2, 3, and 4, in addition to naming the wall, also indicate the relative strength of each wall. It must be emphasized that the walls are not absolute in their compartmentalizing capacities and given enough time, even the barrier zone (Wall 4) will fall. 18

1 Diameter of tree at time of wounding / \ 1 fihji Ijlijil'! Hi- Wood formed after wounding 10-year-old wound Barrier zone Wall 4 Wall 1 Weakest 2 3 4 Strongest 19

ua The type, severity, and position of the wound will affect the extent of compartmentalization. Here are some of the most typical examples. Barrier Wall 4 zone Red maple 20

Three severe basal wounds. All inner compartment walls have fallen and only the barrier zone remains. This is how hollows develop. Barrier zone Wall 4 >\ 21

A basal wound of moderate severity. The entire "group of trees" present at the time of wounding was altered slightly, and were confined by the barrier zone. The side walls, or rays, held here and the column was wedge-shaped in crosssection. The jagged vertical edge was due to variation in confining ability of compartment tops and bottoms in different growth rings. Dark discoloration 22

A slight basal wound. The entire column of wood present at the time of wounding was altered very little, but it was still confined by the barrier zone. The inner walls and side walls held firm here and only a "moon ring" formed. Very faint discoloration Diameter of tree when wounded 23

In general, the same types of columns occur in trees that have a heartwood core. Discolored and decayed wood is compartmentalized in heartwood. When a mechanical wound penetrates the sapwood to the heartwood, the column develops most rapidly along the sapwoodheartwood boundary. Heartwood Heartwood Sapwood Sapwood Wound Young red oak 24

RED Host response to wounding BLUE Surface infection GREEN Discoloration BROWN Decay YELLOW Heartwood Injured cambium Injured cambium Host response njured cambium 25

Heartwood formation stalled near wound. Barrier zone in heartwood 26

Injured cambium Discolored and decayed wood associated with poorly healed large branch stubs is compartmentalized in heartwood. Central columns of defect in heartwoodforming trees are often associated with poorly healed branch stubs. Large broken branches Young oak Wsumfl/ rfp_ Decay 27

Here are the basic patterns of compartmentalized columns of discolored and decayed wood associated with a single wound and with several wounds at one time shown on cross section in trees. nonheartwood-forming 28

Here are some basic patterns for heartwood-forming trees. Discolored heartwood Slightly altered heartwood Ira.. 29

Injured cambium Most trees receive many wounds during their lives. Every tree has some branches that die. When the branches are small and the wounds close rapidly, very little internal defect follows. But, when large branches die and healing is slow, trouble starts for the tree. Add to this the injuries caused by other types of wounds at irregular time intervals and a pattern of multiple columns begins to develop. But again the tree compartmentalizes the injuries and each column is separated from the others. Injured cambium Large broken branch 30

*% Wound Injured cambium, new barrier zone forming Injured cambium 31

Wound Old barrier zone Wall 4 New barrier zone forming Old barrier zone 32

30-year-old branch stub wounds 20-ye. r»rr\oajcrfl( iff^ 33

Open branch stub- Barrier zone Wall 4 Open branch stub A >J Multiple columns are common in trees. A minor wound may set up a central column of discolored wood and later large branches die and heal slowly. The decay associated with the branch stubs does not penetrate the inner column of compartmentalized discolored wood. Diameter when first wounded New column of defect does not move into old central column. Wound 34

A central column of compartmentalized discolored wood may be associated with large branch stubs that healed slowly, but did close before decay set in. Additional columns of discolored and decayed wood could develop later, for example, from severe mechanical wounds on the trunk. Stub Wound Barrier Wall 4 zone 35

Here are some typical patterns of multiple columns found in nonheartwood-forming trees. 4 4 4 mum ^'. If' 36

In heartwood -forming trees the patterns are the same, but they are sometimes difficult to see because they are often contained in heartwood that is already dark in color. Compartmentalization explains how columns of discolored and decayed wood can be found in separated ring patterns by sound wood. 4 4 4 U LL \ w Many columrtsak '»» m> Pmc lm*tl kui* i \ f 37

A major obstacle in understanding multiple columns of compartmentalized decay is the difficulty in "seeing" them in three dimensions. Here are some examples: Birch Column of discoloration and decay associated with a wound developing around a central column of discoloration associated with branch stubs. Barrier zone Central column of discolored wood Stub Old wound 38

Maple Column of discoloration and decay associated with a wound developing around a central column of discoloration. The entire column of wood present at the time of wounding has been altered slightly. When this wood is dried, it will be a different shade from the wood that formed after wounding. Wood altered slightly Central column of discolored wood Wound Barrier zone 39

Pine Column of discolored and decayed wood associated with a wound developing around a central column of discolored heartwood associated with poorly healed branch stubs. Central column of discolored heartwood Sapwood Barrier zone Heartwood Wound 40

Ash Column of discolored and decayed wood associated with a wound developing around a central column of decay associated with old, poorly healed branch stubs. The barrier zone is the ring shake boundary. Barrier zone Ring shake along barrier zone Wound mtcarth IPS 41

j Slightly altered columns of compartmentalized wood associated with wounds in pines are sometimes difficult to see. Some ring patterns of defects in pine form when mechanical wounds are inflicted on trees that already have discolored heartwood. Decay is most advanced along heartwood -sapwood Dejundary. i Wound Heartwood formation stalled. envamh rtfi 42

Another explanation for ring rots in pine and related genera is that some of the decay fungi, such as Fomes pini, first get established in the center of the trunk through branch infections. After establishment, new columns of decay form at the boundaries of the sapwood and heartwood. The new columns are compartmentalized rings. and appear as 43

Old top Sporophore A)- Fomes pini 44

Heartwood Discolored heartwood Sporophore of Fomes pini New column of defect not in sapwood Sporo 45

The "holding power" of columns of discolored wood can be shown by wounds that penetrate the columns. The new column that forms remains separate from the inner columns. When the second wound is severe, decay may develop in the new column. This occurs in nonheartwoodforming trees. New barrier zone Wall 4 Deep drill wound into sapwood and established central column of discolored wood Injured Individual column in each growth cambium ring Discolored column Nonheartwood-forming tree 46

Decay did not penetrate discolored column. I *t>tc3sttp) T72 47

And in heartwood-forming trees. Deep drill wound penetrates sapwood, heartwood, and central column of discolored heartwood. Injured cambium _ btkxuttfi rr?^ When new wounds penetrate old columns of decay, the decay process proceeds rapidly in the new column. -A *»0 48

'>"KztTX>ll r/yz. 49

There are some patterns of defects that on first inspection do not appear to fit the concept of compartmentalization. However, they do. The most notable column begins to develop. An intricate pattern of multiple columns is associated with canker rot. are the defects associated with canker rots. Canker rot fungi, once established in a tree, keep the wound open by slowly killing some living tissues around the wound. This process is the same as re-wounding. And, when the new wound is made, a new New columns form as cambium is killed each year. Some fungi produce sterile fungus material. Diameter of trunk when branch died Fungus kills cambium and new wounds form. 50

! mm hi nmramrv rt?7 51

Ring shake zone Another type of defect that does not appear to fit the concept are ring shakes separation of the wood along the rings. The problem here is that the barrier zone associated with the wounds often forms far beyond the visible column of defect. The barrier zone acts as a partition between the wood present at the time of wounding and the new wood formed after. When growth stresses or other stresses are applied, the wood sometimes pulls apart along the barrier zone. Most shakes are associated with wounds, but not all wounds result in shakes. Slightly altered wood Slightly altered wood Barrier zone Ring "^ shake Large, old open wound Om^tnj, rj fl 52

And, yet another type of defect pattern that appears not to fit the compartmentalization concept is the "island" pattern or streak pattern often spoken of as mineral streak. Wounds indeed start these processes. A pattern type that can be termed "palm and fingers" develops. Near the wound all the columns in the individual growth ring are coalesced to form the "palm." As the discolored columns develop vertically above and below the wound, Walls 1, or the tops and bottoms of the compartments in individual growth rings, react in different degrees to the wound and the invading microorganisms. When such a "palm and finger" column is viewed in cross section at increasing distances above and below the wound, islands of defect appear. Often, a few "fingers" will develop far beyond all the others. BWGMtt ll l-j-^ \if, Wood formed after wounding 53

In sugar maple, for example, the "palm and finger" pattern is the mineral streak pattern associated with sugar maple borer wounds. This insect is a major cause of mineral streak in sugar maple. 54

55

The yellow-bellied sapsucker (see page 7) inflicts several types of wound patterns on many species of trees. In one type of wound pattern a large wound is the result, and the "palm and finger" defect pattern develops. Again, the "fingers" may extend great distances above and below the wound. And cross sections of trunks made through the "fingers" will show islands of defect, or mineral streaks. tw> a/?) 56

\ iv The "palm and finger" defect pattern is also associated with some other wounding patterns made by the sapsuckers. Sapsucker wounds V\ n U flijiifl.fingers is I l *3»k*TTSV- f&* ^caars» /}, 57

*»*» Palm and finger 58

Sapsuckers will often wound one area on a trunk. On paper birch a swollen black band will form at these sites. Not only will discolored streaks of the "palm and finger" pattern develop from such wounds, but the barrier zone that develops after wounding may pull apart from the inner rings to form a complete ring shake which is sometimes called cup shake or loose heart. "'A Amcamil 'f? tmuartt)) rjn. 59

On some trees, such as eastern hemlock, the yellow-bellied sapsucker inflicts many wounds over large areas of the trunk. ""fmrrst/ rift j*% 60

The barrier zones that form after wounding act as partitions between wood present at the time of wounding and wood that forms after wounding. When growth stresses and other stresses develop over long periods, the wood may separate along the barrier zones, and multiple ring shakes form. I;i. I'mM iin\im*)i 11$ 61

The "palm and finger" pattern of defect and barrier zones that form shake are commonly associated with wounds made by larger animals such as beavers and porcupines (see page 9 ). When wounds are severe, Walls 1 and 2 may fall to invading microorganisms. * / i?ni?/>r?3 62

Squirrels wound young, smoothbarked trees in several genera (see page 8 ). The typical "palm and finger" defect pattern results. In some species these defects are called mineral streaks. Bite wounds Canker from old wound 63

Insects wound trees (see page 8) and small islands of defects form. Each island of defect is a small "palm and finger" column. The columns usually penetrate only to the depth of the hole made by the insect. Insect hole Tubes from scale insect Scale insect that lives in old insect holes -" «itt#fw*t'/m/t*it* - Insect holes 11. KlA \v_yt^~. j "^/jv^/avvvxy* 1******^'-* ' Birch N "^ 64

When many insects attack a tree at the same time, a barrier zone may develop around the entire tree. All the wood present at the time of wounding will be slightly altered. When dried, the wood present at the time of wounding will be a different shade from the wood that formed after wounding. 65

The cambium miner is a small larva of a type of fly that eats its way down the cambial region f of some trees. The "tracks" of the larvae are compartmentalized as very long narrow streaks of discolored wood within growth rings. 66

On some trees the wounds are not visible. This is common with small basal wounds, especially those caused by fire when the tree was very young and now the healed wound is hidden by forest litter. The barrier zone still forms around such wounds and often results in ring shake. Also, the inrolled callus serves as a weak spot on the tree that may continue to split vertically. Additional cracks may form from the barrier zone outward into the wood that forms after wounding. When the cross section of a trunk with such a pattern of internal defect is viewed above the base, a star-shaped pattern of cracks radiating out from the center will be seen. 67

With some basal wounds, long internal cracks, called seams, form at right angles to the wounds at the points where the callus inrolls. 68

As these cracks continue to enlarge and get closer to the edge of the trunk, they may suddenly split out to the bark. These secondary seams will be at right angles to the main seam. Most large seams start from old wounds and move outward. frrzcintl? 1972. 69

* ; Seams will also form from mechanical wounds on trunks. Once a seam begins to form, it will usually continue to enlarge v r throughout the life of the tree. i -r-r b \ io.>n\,f~ far ;./ Sn -,>, 70

f f *' * ' //*.-ll 71

In summary, the compartmentalization of defects in trees is a survival system that is effective most of the time not all of the time! And after the tree dies, the powerful decay processes continue to decompose the wood. The decaying wood provides nourishment for a wide variety of organisms.. / iff 72

The decomposed wood provides nourishment for new trees. 73